What Determines the Dielectric Strength of Insulating Oil

Nov 24, 2026

Dielectric strength is the highest electric field an insulating medium can withstand without breaking down. In insulating oil it is not a fixed property of the oil alone. Suspended impurities, moisture, and the way the voltage is applied all change the voltage at which the oil fails.

Breakdown, Breakdown Voltage, and Dielectric Strength

Breakdown is the moment an insulating material forms a path straight through itself under an electric field. A destructive discharge follows, and the voltage between the electrodes falls to zero or close to zero. A solid dielectric loses its dielectric strength permanently. A liquid or a gas loses it only for the moment of the discharge.

Breakdown voltage is the voltage at which a specimen fails under the stated test conditions.

Dielectric strength, also called electric strength, is that breakdown voltage divided by the distance between the electrodes that apply it. The unit is kV/cm.

How Impurities Lower Breakdown Voltage

Impurities in oil come from outside the oil and from breakdown products inside it.

Outside sources are fibers from solid insulation in the equipment, and dust and fibers carried in from the air. Inside the oil, unsaturated hydrocarbons break down into oxides, soluble resins, and sludge. An arc also leaves free carbon, the carbonaceous matter formed when insulating oil decomposes under the arc.

These materials stay suspended through the oil. Under an electric field they line up into a bridge between the electrodes, and the dielectric strength of the oil drops sharply.

How Moisture Lowers Breakdown Voltage

Oil that already holds a lot of suspended matter, or a noticeable amount of free carbon, is also more likely to hold water. Moisture enters as humid air, and it is also released when organic materials inside the equipment, including the oil itself, decompose as the temperature rises.

The hydrocarbons in the oil change how much water it can hold. A higher aromatic content, and a higher temperature, both increase the amount of water the oil can dissolve. That water comes out of solution in microscopic droplets, which adds to the water held in suspension, as an emulsion or as a coarse dispersion, and to the water that stays dissolved.

Moisture lowers the insulation level of the oil, and it has a still larger effect on breakdown voltage. Reported figures show that a water content of only 0.03% already cuts the breakdown voltage by 25%.

Why the Test Conditions Change the Result

Voltage application time

In comparatively clean oil, breakdown voltage has little connection with how long the voltage is applied. Oil used in service always contains some impurities. With those impurities present, a longer time under voltage lowers the breakdown voltage. An AC breakdown test therefore has to specify the rate at which the voltage is raised.

Frequency and waveform

AC breakdown voltage usually rises as the frequency of the applied voltage rises. That rise is an effect of the impurities. Once the impurities are reduced, the link with frequency becomes slight. A higher test frequency weakens ionization in the oil, so the breakdown voltage is higher. At a frequency that is too high, the breakdown voltage falls again: the reactive part of the dielectric loss increases and the oil fails by thermal breakdown.

Waveform matters for the same reason. When the AC wave is distorted, breakdown in most cases follows the peak of the wave, not the rms value. A peaked wave that contains a third harmonic therefore gives a low breakdown voltage when the result is stated as an rms value. Using line voltage as the test supply reduces the effect of harmonics.

Electrode gap

In a uniform field, breakdown voltage is generally proportional to the gap. A field that uniform is obtained only when the gap is very small, 1 mm or less. A larger gap is not a uniform field, even when the electrodes themselves are large. In a non-uniform field, breakdown voltage is not proportional to gap distance.

A result taken at one gap, then scaled to another gap, is not comparable with a result measured at that second gap. The breakdown voltage of oil is always the value at the gap the method specifies.

Electrode shape and material

Shape changes the reading. In comparisons of spherical, spherical-cap, and flat electrodes, spherical electrodes give the highest breakdown voltage, spherical-cap electrodes the next, and flat electrodes the lowest. That order holds for both high and low results. Below 30 kV, the difference between the three shapes tends to shrink.

Surface area matters as well. A larger electrode surface gives a lower breakdown voltage. The account given for this is thermal breakdown: a larger surface weakens convection, so the oil is cooled less, heats faster, and fails at a lower voltage.

Material follows the same thermal picture. At the same gap, the breakdown voltage runs in this order: silver, copper, gold, lead, tin, iron. Silver gives the highest value, copper the next, and iron the lowest. Electrodes made from a material with higher thermal conductivity give a higher breakdown voltage. Test methods therefore specify both the shape and the material of the electrodes.

Temperature

Temperature, moisture, and impurities are the main influences on dielectric strength. Temperature has a stronger effect when the oil already contains impurities and water.

Clean, dry oil depends on its neutral particles remaining unionized. At a given field strength and temperature, those ions are still relatively heavy. If the temperature keeps rising, above about 70 °C to 80 °C, the condition of the molecules changes sharply and the viscosity falls. Ions then accelerate through the oil with little resistance. Collision ionization becomes more likely, and the oil breaks down.

Oil that contains water and impurities behaves differently. At a low temperature the water is suspended as a milky emulsion. Under the field the droplets line up, and electrons pass readily along that bridge, through the volume resistance of the emulsion. The breakdown voltage is low.

As the temperature rises, viscosity falls and the emulsion becomes more mobile. The field disperses it among the neutral molecules of the oil. Viscosity is not yet at its minimum, so the dispersed droplets do not readily rebuild a bridge in the same interval, and the breakdown voltage rises with temperature.

If the temperature keeps climbing until the viscosity reaches a very low value, for example above 70 °C, molecular activity increases. The water droplets can no longer use the drag of the oil to stay clear of the field. They line up again, and the oil breaks down. The temperature at which moist oil reaches its highest breakdown voltage is lower than the corresponding temperature for oil that contains no water.

FAQ

What is the dielectric strength of insulating oil?
It is the highest electric field the oil can withstand without breakdown, calculated as breakdown voltage divided by the electrode gap, in kV/cm.

Why do impurities and moisture reduce breakdown voltage?
Suspended particles and water droplets line up in the electric field and form a conducting bridge between the electrodes.

How much water does it take to change the result?
A water content of 0.03% has been reported to lower the breakdown voltage by 25%.

Why must the electrode gap be specified?
Only a very small gap, 1 mm or less, gives a uniform field in which voltage and gap stay in proportion. Results taken at different gaps are not comparable even after they are scaled to the same distance.

Which electrode shape reads highest?
Spherical electrodes read highest, spherical-cap electrodes next, and flat electrodes lowest. Below 30 kV the difference narrows.